Test method for coating amount of PTP aluminum foil protective agent

Test method for coating amount of PTP aluminum foil protective agent

2022-12-12

Test method for coating amount of PTP aluminum foil protective agent

The protective agent layer of PTP aluminum foil is a dense cross-linked resin layer formed by high temperature curing. It is difficult to completely wipe the coating in a short time by the solvent wiping method commonly used now, and it is difficult to obtain accurate coating quantity value. Moreover, the repeatability of sample test results is also very poor. Therefore, a more effective test method for the coating quantity of PTP aluminum foil protective layer is found, It is of great practical value to guide the production of such products.

According to the material characteristics of PTP aluminum foil and the comparison of the advantages and disadvantages of various detection methods, we finally believe that the "burning method" is the most suitable for the rapid detection of the amount of protective agent coating:

In this method, the PTP aluminum foil sample is placed in a muffle furnace, maintained at a certain temperature for a certain time, and the PTP aluminum foil coated with the protective agent layer is baked at high temperature, so that the protective agent layer is completely oxidized and gasified. The coating amount of the protective agent layer can be calculated by detecting the quality of the aluminum foil before and after the high-temperature baking.

1、 Instruments and reagents:

10cm * 10cm standard cutting plate, blade, analytical balance (precision: 1/10000 g), muffle furnace, glass plate, stainless steel tweezers, ethyl acetate (analytical pure), absorbent cotton

2、 Test method:

1. Select the aluminum foil sample sheet for drug packaging with flat surface and no wrinkles, cut 5 test samples with a blade and a 10cm * 10cm standard cutting plate, and control the deviation of the width and length of the sample within ± 0.5mm

2. Weigh the cut sample (W1) on the balance.

3. Put the printing face of the aluminum foil on a glass plate, and use stainless steel tweezers to clamp the degreased cotton dipped in ethyl acetate to wipe the heat-sealing coating surface of the aluminum foil until no obvious marks can be identified when the surface is observed with naked eyes. (Note: The cotton ball dipped with ethyl acetate shall not have the liquid of ethyl acetate dripping. The circular wiping method from the center to the edge shall be used for wiping. The edge of the aluminum foil must be laid flat on the glass plate, and the linear wiping method shall be used for wiping. The other side of the aluminum foil shall not be affected during the whole process as much as possible). If the cotton ball has been wiped with the printing coating, replace it with a new cotton ball.

4. After wiping the heat-sealing coating, put the aluminum foil in a ventilated place and place it at room temperature for 2 minutes.

5. Then weigh the weight (W2) on the analytical balance

6. Place the above aluminum foil on the sample shelf in the muffle furnace preheated to 550-600 ℃. After waiting for a period of time, take out the coated aluminum foil and place it at room temperature. (The black ink may not completely volatilize the pigment, and its impact can be temporarily ignored for the products with general printed text patterns. If the printed patterns are large, the weight impact of the ink binder and the pigment should be considered)

7. Then weigh the weight (W3) on the analytical balance

Note: If the test sample has no adhesive layer, omit the operations in 2, 3 and 4.

8. Result calculation:

(W1-W2) × 100=weight of heat seal layer (g/m2)

(W2-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has adhesive layer)

(W1-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has no adhesive layer)

W3 × 100=weight of aluminum foil layer (g/m2)

Calculate and report the test results and average values of all individual samples to the nearest 0.01g/m2.


日本在线 一区 二区| 亚洲熟女精品一区二区成人| 亚洲国产精品av在线观看| 欧美精品亚洲精品日韩精品| 亚洲欧洲一区二区综合精品| 人妻内射精品一区二区| 太香蕉久久国产精品视频| 日韩午夜福利高清在线观看| 人妻熟女欲求不满一区二区| 综合久综合久综合久久| 精品一区二区三区不卡少妇av| 国产超碰在线观看免费| 成人日韩视频中文字幕| 亚洲天堂精品一区二区| 伊人色综合久久伊人婷婷| 国产高清三级视频在线观看| 亚洲品质一区二区三区| 91亚洲国产—区=区a| 国产精品不卡免费视频| 色鬼综合久久鬼色88| 国产成人亚洲综合色就色| 欧美成人一区二区三区在线| 97人妻人人揉人人躁人人| 国产精品制服丝袜美腿丝袜| 久久婷婷综合色拍亚洲| 色哟哟哟在线观看视频| 在线观看那种视频你懂的| 国产精品免费视频专区| 好吊色免费在线观看视频| 午夜精品国产精品久久久| 黄色激情视频中文字幕| 日韩特级黄色大片在线观看| 午夜精品麻豆视频91| 亚洲精品有码中文字幕在线观看| 久久中文字幕中文字幕中文| 欧美一区二区三区视频区| 亚洲精品国产主播一区| 91精品日本在线视频| 亚洲精选91福利在线观看| 中文字幕日韩一区二区不卡 | 永久福利盒子日韩日韩|